In-situ, time resolved monitoring of uranium in BFS:OPC grout. Part 1: Corrosion in water vapour.

<p>Uranium encapsulated in grout was exposed to water vapour for extended periods of time. Through synchrotron x-ray powder diffraction and tomography measurements, uranium dioxide was determined the dominant corrosion product over a 50-week time period.  The oxide growth rate initiated rapidly, with rates comparable to the U + H<sub>2</sub>O reaction. Over time, the reaction rate decreased and eventually plateaued to a rate similar to the U + H<sub>2</sub>O + O<sub>2</sub> reaction. This behaviour was not attributed to oxygen ingress, but instead the decreasing permeability of the grout, limiting oxidising species access to the metal surface.</p>